【专家解说】:塑料的防火认证最高级是5VA,申请5VA周期很长,费用很高,如果材料不行还过不了。
根据UL94标准判定材料的难燃性水平。按照HB、V-2、V-1、V-0的顺序,难燃性依次增大。一般说的难燃材料指的是V-0。除了传统的评价方法之外,还设定了上一级的5V评价。作为定位,难燃性顺序依次为V-0、5VB、5VA。由于5V评价的 试验 方法与传统相比有些不同,所以卡中象"V-0、5VA"那样就表示进行了两个 试验 。难燃性 HB < V-2 < V-1 < V-0 < 5VB < 5VA
UL94 5VA & 5VB Flammability Standard
Specimens
Bars: Length 125 mm (5 in) x Width 13 mm (0.5 in) x Thickness [typically 3.0 mm (1
/8 in)].
Plaques: Length 150 mm (6 in) x 150 mm (6 in) x Thickness [typically 3.0 mm (1
/8 in)].
Procedure for Bars
1.A total of 10 specimens (2 sets) are tested per thickness.
2.Five specimens of each thickness are tested after co
nditioning for 48 hours at 23 degrees C and 50% RH.
3.Five specimens of each thickness are tested after co
nditioning for 7 days at 70 degrees C.
4.For bar specimens, the specimens are mounted with the long axis vertical.
5.A 125 mm overall high Bunsen burner flame with a 40 mm blue inner cone is applied to the lower corner of each specimen at an angle of 20 degrees from vertical such that the tip of the blue inner cone touches the specimen. The flame is applied for 5 seco
nds and removed for 5 seconds. The operation is to be repeated until each specimen has been subjected to 5 applications of the test flame.
Procedure for Plaques
Same as for bars except that the plaques are to be mounted on the horizo
ntal plane with the flame applied to the center of the bottom surface of the plaque.
Requirements for 5VA
1.The specimens may not burn with flaming or glowing combustion for more than 60 seco
nds after the fifth application of the test flame.
2.The specimens may not drip flaming particles that ignite the dry absorbent surgical cotton located 300 mm below the test specimen.
3.Plaque specimens may not exhibit burnthrough.
Requirements for 5VB
1.The specimens may not burn with flaming or glowing combustion for more than 60 seco
nds after the fifth application of the test flame.
2.The specimens may not drip flaming particles that ignite the dry absorbent surgical cotton located 300 mm below the test specimen.
3.Plaque specimens can exhibit burnthrough.